Date
|
Experimenter
|
Description
|
Comments
|
10/XX/2017 |
Tanja |
Visual Inspection |
Documentation of crystal's conditions as it arrived at CUA.
|
10/XX/2017 |
Tanja |
Thermal annealing |
Ramp up at 18oC/hour up to 200oC. Stay for 10 hours and ramp down at 18oC/hour.
|
10/XX/2017 |
Tanja |
Longitudinal Transmittance Scan |
Wavelengths: 200-800nm.
|
10/X/2017 |
Tanja |
Wrapped |
Preparing for light yield measurement. 3 layers of teflon tape, and 2 layers of black tape.
|
10/XX/2017 |
Tanja |
LY scan |
Measurement of LY along crystal. More details in the LOGBOOK, runs xx..
Pictures 10/XX/2017
Longitudinal and Transverse Transmittance (TT)
TT (Spectral)
TT (uniformity)
Light Yield
Radiation Hardness
|